1. Belt Splicing
Splices are the weakest section of a conveyor belt. The belt carcass construction determines which joint methods are permitted.
2. Splice Types
| Splice Type | Joint Mechanism | Belt Constructions | Static Strength | Installation and Cure | Principal Limitations |
|---|---|---|---|---|---|
| Hot vulcanised stepped | Plies cut into matching steps, overlapped with tie-gum and cured under heat and pressure | Multi-ply fabric: polyester-polyamide (EP, PN) and polyamide-polyamide (NN) | Typically (N - 1) / N of belt strength, where N is the number of plies, e.g. 67% for 3 plies and 75% for 4 plies. Varies with belt construction and splice design. Confirm with the belt manufacturer. | Heated press, power supply and trained crew. Total downtime including preparation and cooling can exceed 24 h. | Requires a press and power at the splice location |
| Cold vulcanised stepped | Same step geometry bonded with two-part polychloroprene cement at ambient temperature, without a press | Multi-ply fabric, lower tension | Lower than hot vulcanised. Sensitive to workmanship and cure conditions. | No press. Typically 4 h for a usable cure and 24 h for full cure. | Lower heat resistance. Standard cements may not bond to heat-resistant covers. |
| Finger, thermoplastic fused | Interlocking fingers fused with polyvinyl chloride (PVC) plastisol or polyurethane jointing paste in a heated press | Solid woven PVC | Belt manufacturer rating | Single press setting. Held under pressure until below 70 deg C [158 deg F]. | Requires templates, punches and a press sized for the full splice |
| Finger, vulcanised | Interlocking fingers bonded with tie-gum and vulcanised | Solid woven PVC with nitrile rubber covers (PVG), single-ply straight-warp and aramid. Some high-tension multi-ply fabric designs. | Belt manufacturer rating | Single press setting | Manufacturer-specific geometry and materials |
| Steel cord overlap | Cords from each belt end overlap in core rubber. Load transfers between cords by rubber shear. | Steel cord | Up to 100% of nominal belt strength when correctly made | Single press setting. Splice length typically 0.6 m [2 ft] at ST 1000 to 4.5 m [15 ft] at ST 5400, longer at higher ratings. | Sensitive to workmanship. Verify internal geometry by radiography or magnetic flux leakage (MFL) scan. Apply High Integrity Splicing (HIS) on high-tension belts. |
| Mechanical fastener | Hinged or solid plate fasteners clamped, bolted or riveted through the belt ends | Multi-ply fabric, typically up to EP 1000. Solid woven. | Fastener manufacturer rating. Typically derate working tension by 20% to 25% relative to a vulcanised splice. | No cure. Shortest downtime. | Unsuitable for steel cord. Exposed to cleaner and impact damage. Metallic fasteners trip metal detectors unless the detector logic masks the splice. Joint gaps can pass fines. |
Note: Static strength does not govern splice life. DIN 22101 bases belt and splice selection on the dynamic splice efficiency, determined by fatigue testing to DIN 22110-3, which is lower than the static strength.
3. Hot Vulcanised Stepped Splices (Multi-Ply Fabric)
Multi-ply fabric belts (EP, PN and NN) are joined with a stepped splice of N - 1 steps, where N is the number of plies, vulcanised under heat and pressure.
| Step | Action | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| 1. Mark out | Align the belt ends on the true belt centreline. Mark the bias and step lines. | Bias length 0.3 times belt width, or 0.4 times where specified. Step length set by the strength of each ply, to the belt manufacturer's splice instructions. | A square splice concentrates dynamic stress at pulleys, idlers and cleaners. Short steps reduce bonded area. |
| 2. Strip and step | At each step line, cut through the cover and the ply being removed, then peel that ply from the skim rubber. Use induction cover heaters and stripping winches where available. | Do not score the ply beneath | A cut into an underlying ply reduces its strength across the full splice |
| 3. Buff and clean | Buff all bonding surfaces to a uniform texture. Clean with the manufacturer's solvent, typically ethyl acetate or methyl ethyl ketone (MEK). | Do not overheat the rubber. Do not use degreasers, mineral spirits or unfiltered compressed air. Control ignition sources, as both solvents are flammable. Substrate temperature at least 3 deg C [5 deg F] above the dew point. | Scorched or contaminated surfaces bond poorly. Condensation vaporises during cure and leaves voids. |
| 4. Assemble | Apply cement and tie-gum, lay the steps together and rebuild the covers with cover compound of the belt cover grade | Materials within shelf life, typically 6 months at 21 deg C [70 deg F] or 12 months at 10 deg C [50 deg F]. Do not use tie-gum as cover rubber. | Aged compound flows poorly during cure. Tie-gum covers have lower abrasion resistance than cover compound. |
| 5. Cure | Cure in a heated press. Long splices can be cured in more than one press setting. | Temperature, pressure and time to the manufacturer's cure table for belt thickness and compound | Under-cure. Over-cure at press overlaps. |
| 6. Cool and release | Hold full press pressure until the splice cools to approximately 70 deg C [158 deg F], or the manufacturer's release temperature, then release | Do not tension the belt until the press is removed | Blistering and porosity |
| 7. Finish and inspect | Grind flash and surplus rubber flush with the belt. Inspect for voids, edge lifting and alignment. | Splice thickness matches the parent belt | A proud splice strikes cleaners and causes thumping |
4. Cold Vulcanised Stepped Splices (Multi-Ply Fabric)
Cold splicing uses the stepped splice geometry bonded with two-part polychloroprene cement at ambient temperature, without a press. Use it on lower-tension fabric belts within the cold-bond system manufacturer's rating.
| Step | Action | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| 1. Mark out and step | Mark the bias and step lines, cut and peel the plies | Bias 0.3 or 0.4 times belt width. Step length set by ply strength. Do not score the ply beneath. | Damaged plies and reduced bonded area |
| 2. Buff | Buff all bonding surfaces to a uniform texture | Without heat and pressure, adhesion depends on mechanical key | Weak bond |
| 3. Clean and check conditions | Clean with the manufacturer's solvent | Substrate temperature at least 3 deg C [5 deg F] above the dew point. Confirm cement compatibility with heat-resistant cover compounds. | Condensation or an incompatible compound reduces adhesion |
| 4. Cement | Mix the base cement and hardener and apply to both surfaces | Use within the manufacturer's open time and expiry date | Aged cement bonds poorly |
| 5. Assemble | Join the steps, roll out entrapped air and rebuild the covers. Apply weight over the splice during cure. | Uniform contact across the full splice | Entrapped air and unbonded areas |
| 6. Cure | Hold the conveyor stopped through the cure period | Typically 4 h for a usable cure and 24 h for full cure, depending on cement formulation and ambient temperature. Apply the manufacturer's cure time. | Loading before cure shears the bond |
Note: Cold splices have lower heat resistance than hot vulcanised splices and degrade faster on hot materials such as cement clinker, foundry sand and hot ash.
5. Finger Splices
Finger splices join belts that cannot be stepped: solid woven PVC and PVG, single-ply straight-warp and aramid belts. They also join some high-tension multi-ply fabric designs.
| Step | Action | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| 1. Mark out | Mark the fingers with steel templates. Set the splice square or on a bias as the belt manufacturer specifies. | Finger length to the belt manufacturer's splice instructions | Short fingers reduce shear area and joint strength |
| 2. Cut fingers | Cut with heavy-duty saws or pneumatic punches | Do not cut fingers by hand | Irregular gaps between fingers disrupt tension transfer |
| 3. Prepare surfaces | Buff and clean the finger edges for vulcanised splices | Substrate temperature at least 3 deg C [5 deg F] above the dew point | Poor adhesion and voids |
| 4. Fill and interlock | PVC: apply plastisol or jointing paste between the fingers. PVG, straight-warp and aramid: apply tie-gum. Interlock the fingers. | Fill every finger gap | Unfilled gaps carry no shear |
| 5. Cure | Cure the full splice in a single press setting | Temperature, pressure and time to the manufacturer's cure table | Plastisol or rubber flow and finger displacement at a press overlap |
| 6. Cool and release | Hold full press pressure until the joint cools below 70 deg C [158 deg F]. Water-cooled platens shorten the cooling time. | Confirm release temperature at the platens | Weak, porous joint |
| 7. Finish and inspect | Trim flash. Check finger alignment and joint thickness. | Joint thickness matches the parent belt | Uneven joint strikes cleaners |
6. Steel Cord Splices
Steel cord belts are joined only by hot vulcanised overlap splices. Use the belt manufacturer's splice design to ISO 15236-4 (formerly DIN 22131-4).
| Step | Action | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| 1. Align and mark | Overlap the belt ends, align them on the true belt centreline and mark the bias | Bias 0.3 times belt width or 0.4 times, unless the splice design specifies a square splice | A misaligned splice mistracks |
| 2. Strip and clean cords | Strip the covers with motorised cord strippers and induction cover heaters. Clean with the manufacturer's solvent. | Hold the blade inclined toward the cover to leave a core rubber film on each cord. Do not buff or score through the zinc coating. Substrate temperature at least 3 deg C [5 deg F] above the dew point. | Low cord-to-rubber adhesion |
| 3. Cut and lay cords | Cut the cords to the lengths in the splice diagram and lay them in the step pattern | Staggered cord ends. Number of steps and step length to the splice design. Step count rises with cord diameter relative to cord pitch. Typically 1 step up to ST 1600 or ST 2000 and 4 steps from ST 5000 to ST 7500. Use alignment combs to hold the cords parallel. | Coinciding cord ends concentrate stress. Misaligned cords. |
| 4. Insert core rubber | Lay core rubber strips (noodles) or pre-grooved core rubber panels between the cords | Minimum gap approximately 0.25 times the cord diameter. Typically one third of the cord diameter. | Cord-to-cord contact removes the shear path |
| 5. Build edges and covers | Build the edges with edge rubber and apply the cover rubber | Consolidate the edges fully | Exposed outer cords corrode inward (zipper failure) |
| 6. Cure | Cure the full splice in a single press setting. Tighten traverse beams with calibrated torque wrenches in a set sequence. | Temperature, pressure and time to the manufacturer's cure table, logged | Rubber flow and cord displacement at press overlaps. Voids. |
| 7. Cool and release | Hold full press pressure until the splice cools to approximately 70 deg C [158 deg F], or the manufacturer's release temperature | Do not tension the belt until the press is removed | Blistering and porosity |
| 8. Inspect | Inspect cord geometry by radiography (X-ray) or MFL scan | Cord alignment and core rubber gap to the splice design. Reject any cord-to-cord contact. | Geometry errors reduce static and dynamic splice strength |
7. High Integrity Splicing (HIS)
Apply HIS to high-tension steel cord belts and to belts where splice failure has a high production or safety consequence. HIS adds engineering controls to the steel cord splicing process to reduce variation in field splice quality.
| Control | Requirement | Purpose |
|---|---|---|
| Splicing enclosure | Pressurised enclosure with heating, ventilation and air conditioning (HVAC) | Holds temperature and humidity within the splice material manufacturer's limits. Absorbed moisture vaporises during cure and causes voids. |
| Cord alignment | Laser alignment jigs and machined aluminium combs over the full splice length, which can reach 4 to 5 m [13 to 16 ft] | Keeps the cords parallel and on the splice pattern |
| Core rubber | Pre-grooved core rubber panels in place of hand-laid strips | Holds the design gap between cords |
| Cure control | Digital proportional-integral-derivative (PID) controllers, multi-zone thermocouples and data logging in place of manual gauges | Controls and records the full cure profile against the target |
| Baseline scan | Record a radiograph or MFL scan of every splice after cure | Sets the baseline for condition monitoring |
8. Splice Inspection and Repair
Splices degrade through dynamic fatigue, impact damage and chemical breakdown. Inspect splices routinely by visual, tactile and auditory checks to identify degradation before the belt parts.
8.1 Splice Inspection
| Condition | Indicators | Probable Cause | Corrective Action |
|---|---|---|---|
| Cover blistering or sponginess | Tactile softness or visible surface blistering | Subsurface moisture or air entrapment. Under-cure, or press released before cooling. | Apply a hot vulcanised spot repair where localised. Replace the splice where blistering covers a large area or reaches the carcass. |
| Transverse cracking | Transverse cracks at the leading or trailing splice ends | Abrupt stiffness transition between belt and splice. Pulley diameter below the belt minimum. Square or short splice. | Spot repair cover cracks before moisture enters. Check pulley diameters against the belt manufacturer's minimums. Replace the splice where cracks reach the carcass. |
| Edge fraying and zipper separation | Fabric ply delamination or protruding steel cords at the edge | Outer step shear failure. Edge tension overload transferring to adjacent cords. Edge contact with the structure from mistracking. Poorly consolidated edge rubber. | Correct belt tracking. Rebuild the edge where cords or plies are intact. Replace the splice where cords are broken or corroded. |
| Step edge lifting | Lifted cover or ply edge along a step line, visible as a ridge | Contaminated or under-buffed bond line. Cleaner blade catching the step edge. | Re-bond the lifted edge with tie-gum under a spot press. Check cleaner blade angle and tension. |
| Finger tip separation | Finger tips lifting or cracking along the finger boundaries | Incomplete fusion or bond. Fingers too short. Press released before cooling. | Spot repair isolated tips. Replace the splice where separation extends along the fingers. |
| Hourglassing (necking) | Local reduction in belt width under tension | Internal shear failure, with cords or plies slipping longitudinally | Failure is imminent. Stop the conveyor and replace the splice. |
| Splice elongation | Increase in steel cord splice length between successive MFL scans | Cords pulling through the core rubber under cyclic load | Increase scan frequency. Schedule splice replacement before necking is visible. |
| Protruding steel cords | Cord ends or broken wires visible through the cover | Cord displacement during cure, cover wear or cord fatigue failure | Isolate the conveyor and assess. Replace the splice where cords are broken. |
| Corrosion staining | Rust staining at cover damage on a steel cord splice | Moisture ingress to the cords | Seal the cover with a hot vulcanised spot repair. Scan by MFL to assess cord loss. |
| Thumping | Repetitive impact noise at idlers and cleaners | Splice profile cupped or thicker than the belt | Grind a proud splice flush. Investigate cupping, which can indicate internal separation. |
| Splice mistracking | Belt moves laterally each time the splice passes a pulley | Belt ends not aligned on the true belt centreline, or bias error | Re-make the splice with the belt ends aligned on the true belt centreline |
| Accelerated cover wear | Splice cover thinner than the adjacent belt, or scored | Tie-gum used as cover rubber, wrong cover compound or over-tensioned cleaner | Rebuild the cover with cover compound of the belt grade. Reset cleaner tension. |
| Cold splice heat degradation | Hardened, cracked or debonding cold splice on hot duty | Cold splice operating above its heat resistance | Replace with a hot vulcanised splice |
| Fastener damage | Loose, cupped or broken fastener plates or hinge pins. Carcass tearing along the fastener line. | Fastener undersized for belt thickness, pulley diameter below the fastener minimum, or cleaner impact | Replace damaged fasteners. Re-cut the belt end square and refit where the carcass is torn. Plan a vulcanised splice where damage recurs. |
8.2 Repair Methods
| Method | Description | Application | Limitations |
|---|---|---|---|
| Hot vulcanised spot repair | Route out damaged rubber to the carcass, clean, fill with tie-gum and cover compound, then cure with a spot press | Cover gouges, cracks and blisters, to seal against moisture ingress | Does not restore tensile capacity where cords or fabric are damaged |
| Hot vulcanised edge repair | Remove damaged edge rubber, buff, rebuild with edge rubber and cure with a spot press | Frayed or abraded edges with intact cords or plies. Restores the edge moisture seal on steel cord belts. | Not effective where outer cords are broken or corroded |
| Step edge re-bond | Lift, buff and clean the separated edge, apply tie-gum and cure with a spot press | Localised step edge or finger tip lifting where the internal bond is sound | Not suitable where separation extends into the splice body |
| Cold bond repair | Fill gouges or scuffs with two-part polyurethane compounds or cold-vulcanising cements | Temporary cover repair where a spot press is unavailable. Cure time to the compound manufacturer's instructions. | Limited abrasion resistance. Primary belt cleaners can remove the repair. |
| Grinding flush | Grind proud splice rubber flush with the belt | Thumping and cleaner impact from a thick splice | Does not correct cupping caused by internal separation |
| Mechanical fastener reinforcement | Fit solid plate fasteners across a delaminating fabric splice edge to bind the plies | Short-term contingency on fabric belts only | Do not use on steel cord belts, where fasteners can be ejected under tension |
| Temporary fastened closure | Cut out the failed splice and close the belt with mechanical fasteners | Emergency return to service on fabric and solid woven belts, within the fastener limits for the belt | Derate the working tension. Replace with a vulcanised splice at the next shutdown. Unsuitable for steel cord belts. |
| Single replacement splice | Cut out the failed splice and make one new splice | Permanent repair where take-up travel can absorb the belt length consumed | Consumes belt length. Confirm the remaining take-up travel before cutting. |
| Insert (saddle) splice | Cut out the failed splice, insert a new section of belting and vulcanise two new splices | Permanent repair where take-up travel cannot absorb a single replacement splice. Restores design capacity. | Two splices to make and maintain. Match the insert to the parent belt construction, rating and cover grade. |