1. Belt Manufacturing
Manufacturing processes differ across multi-ply fabric, straight-warp, solid woven polyvinyl chloride (PVC), steel cord, aramid and thermoplastic polyurethane (TPU) constructions.
| Construction Type | Carcass Architecture | Matrix / Elastomer | Curing or Forming Process | Primary Technical Advantage |
|---|---|---|---|---|
| Multi-Ply (EP/NN) | Stacked woven plies with inter-ply skim coats | Vulcanised Rubber | Step Press / Rotary | Versatility across tension ranges and splice methods |
| Straight-Warp | Single integrally woven carcass with uncrimped warp yarns | Vulcanised Rubber | Step Press | Low constructional stretch and high rip propagation resistance |
| Solid Woven (PVC) | Integrally woven carcass with interlocked binder yarns | Thermoplastic PVC | Oven Heat Fusion | No plies to separate. Suited to Fire Resistant Anti-Static (FRAS) certification. |
| Steel Cord (ST) | Longitudinal galvanised steel cords in core rubber | Vulcanised Rubber | Tensioned Step Press | High tensile strength. Low elongation. |
| Aramid | Woven aramid warp and polyamide weft, typically single-ply straight-warp | Vulcanised Rubber | Step Press | High strength-to-mass ratio. Low elongation. Non-magnetic and corrosion resistant. |
| Thermoplastic (TPU) | Pre-tensioned synthetic carcass | Thermoplastic polyurethane | Extrusion coating or lamination | Food-grade compounds available. Chemical resistance and field weldability. |
Note: EP denotes a polyester warp and polyamide (nylon) weft. NN denotes a polyamide warp and weft.
2. Compounding and Adhesion Treatment
Compounding and adhesion treatment are common to all vulcanised rubber constructions. Adhesion between reinforcement and rubber governs delamination resistance and cord pull-out strength.
| Stage or Reinforcement | Process | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| Compounding | Internal mixers blend the base elastomer with carbon black, curatives (sulphur or peroxide), accelerators, antioxidants and plasticisers. Base elastomers include natural rubber (NR), styrene-butadiene rubber (SBR), nitrile rubber (NBR) and ethylene propylene diene monomer (EPDM). The uncured compound is sheeted for calendering. | Mix temperature and time. Cure characteristics verified by rheometer. | Premature cure (scorch). Inconsistent cover properties. |
| Polyamide fabric | Dipped in resorcinol formaldehyde latex (RFL), dried and heat-set under tension. The RFL co-vulcanises with the rubber. | Dip pick-up and cure temperature | Low ply and cover adhesion |
| Polyester and aramid fabric | Adhesion-activating pre-dip (epoxy or blocked isocyanate) followed by RFL, or adhesive-activated polyester yarn with a single RFL dip. RFL alone on untreated yarn gives inadequate adhesion to polyester and aramid. | Pre-dip chemistry and cure temperature | Ply separation and cover delamination |
| Steel cord | Galvanised cords bond directly to a core rubber formulated for adhesion to galvanised steel. | Cord surface cleanliness. Core compound adhesion system. | Low cord pull-out strength |
RFL-free adhesive systems eliminate resorcinol and formaldehyde. Request long-term adhesion data from the manufacturer before specifying RFL-free fabric.
3. Multi-Ply Fabric Belting
Multi-ply belts are built from separately calendered fabric plies bonded by rubber skim coats and cured as a single assembly.
| Stage | Process | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| Calendering | Heated calender rolls force uncured rubber into the fabric weave (frictioning). A second pass applies a skim coat that forms the inter-ply bond. Four-roll calenders coat both faces in a single pass. | Roll temperature, speed ratio and skim thickness | Low ply adhesion. Entrapped air. |
| Lay-up | The bottom cover, plies and top cover are stacked on a building table and consolidated by pressure rolls. | Ply alignment and air expulsion | Camber, edge wander and blisters |
| Vulcanisation | Hydraulic step press in sequential press lengths, or continuous rotary press, at typically 140 to 160 deg C [284 to 320 deg F]. Specific pressure and dwell time are set for the compound and belt thickness. | Platen temperature uniformity, pressure, dwell time and press-length overlap | Under-cure. Over-cure at overlaps. Thickness variation. |
| Press Type | Mechanism | Application | Advantages | Limitations |
|---|---|---|---|---|
| Flat step press | Heated steel platens under hydraulic pressure. The belt is indexed through in press lengths. | Fabric and steel cord belts | High pressure. Accommodates thick belts and cord pre-tensioning. | Overlap zones between press lengths risk over-cure |
| Continuous rotary press | The belt is held against a heated rotating drum by a tensioned steel band | Fabric belts | Continuous cure without overlap zones. Uniform thickness. | Maximum belt thickness is limited. Confirm with the manufacturer. Not suited to steel cord pre-tensioning. |
4. Straight-Warp and Aramid Belting
Straight-warp belts carry load on uncrimped warp yarns in a single integrally woven carcass, which reduces constructional stretch and yarn-on-yarn abrasion and improves rip propagation resistance and impact fatigue life. Aramid belts are manufactured by the same process.
| Stage | Process | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| Weaving | Heavy warp yarns (polyester, polyamide or aramid) are held flat and parallel. Weft yarns are inserted across the width, and binder yarns pass through the full thickness to lock the structure. Aramid constructions use a polyamide weft and binder. Carcass thickness increases with the number of warp layers and yarn linear density. | Warp tension uniformity | Camber. Uneven load sharing between warp yarns. |
| Calendering | The complete fabric is calendered on both faces. Rubber penetrates the warp spacing and binder structure during press curing. | Rubber flow and penetration | Dry carcass core. Low cover adhesion. |
| Lay-up | Top and bottom covers are applied and consolidated. No ply stacking is required. | Cover thickness and air expulsion | Blisters. Cover thickness variation. |
| Vulcanisation | Flat hydraulic step press. Dwell is set by carcass thickness to cure the core fully. | Cure profile, so that the core reaches full cure before the covers over-cure | Under-cured core. Over-cured covers. |
5. Solid Woven PVC Belting
Solid woven belts have an integrally woven carcass saturated with PVC and fused by heat. The interlocked weave has no plies to separate, and the construction is widely used for FRAS-certified underground coal belting.
| Stage | Process | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| Weaving | A three-dimensional loom weaves polyester or polyamide warp yarns, polyamide weft yarns and binder yarns into a single interlocked carcass. Carcass thickness is typically 5 to 15 mm [0.2 to 0.6 in] for 400 to 1,800 kN/m [2,300 to 10,300 PIW]. Cotton binder yarns absorb plastisol and improve PVC bonding and fastener retention. All-synthetic binders reduce moisture absorption and resist biological degradation. | Weave density and binder interlock | Low fastener retention. Weave distortion. |
| Impregnation | The carcass is impregnated with PVC plastisol by vacuum impregnation after weaving, or by wet weaving, in which the warp yarns are impregnated during or before weaving. Full core saturation of the dense carcass is the primary process difficulty. | Core saturation | Dry core. Internal moisture wicking. |
| Gelling and fusion | A multi-zone oven (infrared and forced convection) at typically 160 to 200 deg C [320 to 390 deg F] fuses the plastisol into a solid thermoplastic matrix. The carcass is held under controlled tension to set the final belt elongation. | Oven temperature profile, line speed and carcass tension | Incomplete fusion. Low matrix strength. PVC degradation at excess temperature. High belt elongation. |
| Covers | PVC covers are coated onto the impregnated carcass, gelled and pressed. PVC and nitrile rubber blend (PVG) covers are used where higher drive friction and abrasion resistance are required. Nitrile is compatible with PVC and fuses to the impregnated carcass in a press. | Cover-to-carcass adhesion | Cover delamination |
FRAS certification applies to the complete belt construction. A change of binder yarn, impregnation compound or cover compound requires recertification. For underground belts, request sectioned samples demonstrating full core impregnation.
6. Steel Cord Belting
Steel cord belts have a single layer of longitudinal galvanised steel cords embedded in core rubber. Without a woven carcass, cord tension and position during manufacture govern belt straightness and tracking.
| Stage | Process | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| Creel tensioning | Each cord is unwound from a creel and tensioned to the production tension. Individual cord tension measurement and control improve tension uniformity across the width. | Cord tension uniformity across the width | Locked-in stress, camber and mistracking |
| Core calendering | A machined comb sets the cord pitch. Top and bottom layers of uncured core rubber are applied, penetrating between and into the cords. | Cord pitch and rubber penetration | Cord contact. Low pull-out strength. Internal corrosion paths. |
| Lay-up | Covers, edge rubber and any rip detection loops or transverse breakers are applied. | Cover thickness and edge build | Thin covers. Exposed edge cords. |
| Vulcanisation | Flat hydraulic step press. The cords are clamped and held under tension while the press closes and the rubber cures. Continuous rotary curing is rarely used because uniform cord tension and cord position are difficult to maintain around a drum. | Cord pre-tension, platen temperature and press-length overlap | Camber, cord waviness and over-cure at overlaps |
For wide or high-tension belts, state the creel tension control method and the X-ray acceptance criteria for cord pitch and broken cords in the purchase specification.
7. Thermoplastic Polyurethane Belting
TPU belts are thin, low-tension constructions with limited impact capacity, used in food processing, packaging and logistics. They are generally outside the scope of heavy-duty bulk materials handling.
| Stage | Process | Critical Controls | Defect if Uncontrolled |
|---|---|---|---|
| Coating | Molten TPU is extrusion-coated onto a pre-tensioned polyester or aramid fabric, or TPU film is laminated under heat and pressure. No vulcanisation is required. | Coating thickness and fabric tension | Coating thickness variation. Camber. |
| Splicing | Hot-bar or hot-air welding | Weld temperature and dwell time | Low joint strength |
8. Edge Finishing
Select the edge finish to suit the operating environment. Steel cord belts are manufactured with moulded edges to protect the outer cords from corrosion.
| Edge Type | Manufacturing Process | Cost / Throughput | Environmental Isolation | Recommended Application |
|---|---|---|---|---|
| Cut Edge (Slit) | Master roll slit by rotary knives after vulcanisation | Low cost / high throughput | Low (exposed plies susceptible to moisture wicking) | Dry service |
| Moulded Edge | Built to final width. Edges rubber-encapsulated and press-moulded. | High cost / low throughput | High (sealed carcass) | Corrosive, acidic or wet environments |
| Sealed Cut Edge | Slit edge coated with liquid polymer sealant and cured | Moderate cost / moderate throughput | Moderate (thin barrier, susceptible to mechanical abrasion) | Moderately humid environments requiring baseline protection |
9. Factory Acceptance Testing
Factory Acceptance Testing (FAT) verifies finished belt integrity against the purchase specification. Manufacturing defects, including uneven cord tension, entrapped air and incorrect cure, cannot be rectified in situ and shorten belt life.
State the required tests, sampling frequency and acceptance criteria in the purchase specification. Destructive tests are performed on samples cut from the belt before shipment.
| Test Protocol | Applicable Standard(s) | Technical Objective |
|---|---|---|
| Abrasion Resistance | ISO 4649 (formerly DIN 53516) | Quantifies cover volume loss under controlled abrasion. |
| Total and Cover Thickness | ISO 583 (fabric) / ISO 7590 (steel cord) | Verifies total and cover thickness against the specified tolerances. |
| Peel Adhesion | ISO 252 (fabric) / ISO 8094 (steel cord cover to core) | Verifies cover-to-carcass and ply-to-ply adhesion. |
| Full-Thickness Tensile Strength | ISO 283 (fabric) / ISO 7622-2 (steel cord) | Verifies full-thickness breaking strength. |
| Elongation at Break and Reference Load | ISO 283 (fabric) / ISO 7622-1 (steel cord) | Measures carcass elongation at break and at reference load. |
| Troughability | ISO 703 | Measures transverse flexibility to confirm the belt conforms to the trough. |
| Rheometric Cure Analysis | ISO 6502 series | Measures compound cure characteristics (scorch time, cure rate and state of cure) by rheometer. |
| Cover Hardness | ISO 48-4 (Shore A) | Measures cover hardness. |
| Tear Resistance | ISO 34-1 | Measures tear propagation force in the cover compound. |
| Cord Pull-Out Adhesion | ISO 7623 | Measures the force to extract a cord from the core rubber (steel cord belts only). |
| Electrical Surface Resistance | ISO 284 | Verifies anti-static performance. |
| Flammability | ISO 340 | Measures flame retardance at laboratory scale. Grade S FRAS certification to AS 4606 additionally requires drum friction and large-scale combustion propagation (gallery) tests. |
Note: Electrical surface resistance and flammability tests are required where anti-static or fire-resistant performance is specified.